ST52.3 High Strength Structural Steel
ST52.3 is a high-strength, low-carbon manganese structural steel formerly specified under the German DIN 17100 standard. It is characterised by its excellent combination of strength, toughness, weldability and machinability, making it suitable for a wide range of demanding engineering and structural applications. With a minimum yield strength of approximately 355 MPa in smaller sections, ST52.3 offers higher load-bearing capacity than conventional mild steel while retaining good fabrication properties.
ST52.3 is generally supplied in the as-rolled or normalized condition. Its controlled carbon content and manganese composition contribute to its good weldability and mechanical strength. The material also provides good impact resistance and can be used in components subjected to both static and dynamic loading. Its machinability is generally comparable to that of mild steel, making it suitable for various machining and fabrication processes.
ST52.3 is widely used across the engineering, construction and manufacturing industries for components requiring a combination of high strength, durability and reliable performance.
Typical uses are: Machine Frames, Hydraulic Cylinder Components, Structural Supports, Connecting Rods, Mounting Plates, Industrial Machinery Components, Welded Assemblies, Heavy-Duty Brackets, Base Plates, Load-Bearing Structures and General Engineering Components.
Equivalent Grades – ST52.3
| EU EN |
USA – |
Germany DIN,WNr |
Japan JIS |
France AFNOR |
England BS |
Italy UNI |
Spain UNE |
China GB |
Sweden SS |
Poland PN |
Czechia CSN |
Austria ONORM |
Russia GOST |
Inter ISO |
| S355J2G3 | A572 Gr.50 | ST52-3 / 1.0570 | SM53C | E36-4 | 50D | Fe510-D | A510D | Q355B* | 2134-01 | — | — | St510D | S345 | Fe510-D |
Available Types & Range
Available Types & Range
C 40 steel Supply Form & Size
| Form of Supply | Size(mm) | Length(mm) |
| Round bar | Φ20-Φ650 | Standard or As your request |
| Square bar | 25 x 25 – 450 x 450 | Standard or As your request |
| Plate/Sheet | Thickness :6 – 300 Width:80-1,250 |
Standard or As your request |
| Flat bar/Blcoks | Thickness :10 – 300 Width:120-25 – 500 |
Standard or As your request |
Related Specifications
Chemical Composition
Chemical Composition & Technical Specification -C 40
| Grade | C | Si | Mn | P | S |
| C40/1.0511 | 0.20 | 0.55 | 1.60 | 0.040 | 0.040 |
Typical Mechanical Properties – As Rolled
| Tensile Strength Mpa | 490–630 | |
| Yield Strength Mpa | 315–355 | |
| Elongation on 5.65√S0 % | 18–22 | |
| Hardness | HB | Approx. 150–190 |
| Rc | Not specified |
Forging
Heat to 900°C–1150°C and allow the temperature to become uniform throughout the section before commencing forging. Hot forging should be carried out within the recommended temperature range. Avoid excessive soaking at high temperatures, as this may cause grain growth and surface scaling.
Forging should be completed before the material temperature falls below approximately 850°C. Following completion of forging, the workpiece should be cooled under controlled conditions.
| Heat Treatment |
|
Soft Annealing |
|
Heat to 650°C–700°C, hold until the temperature is uniform throughout the section, and cool slowly. |
| Hardening |
| Refer Refining & Hardening. |
| Normalizing |
|
Conventional through-hardening is not normally recommended for ST52.3 as it is a low-carbon structural steel. It is primarily supplied and used in its structural delivery condition. |
| Refining & Hardening |
| Stress Relieving | ||||
|
Heat to 550°C–580°C after heavy machining or welding, allow the temperature to become uniform throughout the section, and hold for approximately 4 hours. Cool slowly to minimise the introduction of additional residual stresses. |
||||
| Tempering | ||||
|
Tempering is not normally required for ST52.3 supplied in its standard structural condition. If a specialist hardening treatment is carried out, the tempering temperature and holding time should be determined by the heat-treatment specialist according to the required properties. |
||||
| Notes on Heat Treatment | ||||
|
ST52.3 is generally supplied in the as-rolled or normalized condition and does not normally require additional heat treatment. Heat-treatment requirements depend on the material condition, component dimensions, machining operations and intended application. Heating temperatures, holding times and cooling rates should be established by a qualified heat-treatment specialist. Consult the material supplier and heat treater before carrying out any heat-treatment operation. |
||||
| Machining | ||||
|
ST52.3 has good to very good machinability and is suitable for conventional machining operations such as turning, drilling, milling and tapping. Suitable cutting tools, feeds and speeds should be selected according to the material condition, component dimensions and machine manufacturer’s recommendations. |
||||
| Welding | ||||
|
ST52.3 is readily weldable in its as-rolled or normalized condition using conventional welding processes. It is suitable for common fabrication methods, including Manual Metal Arc (MMA), Metal Inert Gas / Metal Active Gas (MIG/MAG) and Submerged Arc Welding (SAW). Welding should be carried out using suitable compatible filler materials. Low-hydrogen consumables are recommended, particularly for thicker sections and highly restrained joints. |
||||
| Welding Procedurde | ||||
|
Welding procedures should be selected according to material thickness, joint design, welding process and service requirements. Suitable welding consumables should be selected to provide the required strength and toughness of the welded joint. |
||||
| Post Welding | ||||
|
Allow the welded component to cool naturally under controlled conditions. Avoid rapid cooling or water quenching. Post-weld stress relieving is not normally required for standard structural applications. Where required due to heavy machining, complex geometry or specific fabrication requirements, a suitable stress-relieving procedure should be established by a qualified specialist. |